Surface Chemistry of Copper Precursors in Connection with Atomic Layer Deposition (ALD) Processes
|
|
- Gordon Clark
- 6 years ago
- Views:
Transcription
1 Surface hemistry of opper Precursors in onnection with Atomic Layer Deposition (ALD) Processes The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters. itation Accessed itable Link Terms of Use Ma, Qiang, Roy G. Gordon and Surface chemistry of copper precursors in connection with atomic layer deposition (ALD) processes. Paper presented at The 11th International onference on Atomic Layer Deposition, ambridge, MA, June 26-29, May 13, :46:40 AM EDT This article was downloaded from Harvard University's DASH repository, and is made available under the terms and conditions applicable to Other Posted Material, as set forth at (Article begins on next page)
2 Surface hemistry of opper Precursors in onnection with Atomic Layer Deposition (ALD) Processes Qiang Ma, Roy G. Gordon 1, and Dept. hemistry, University of alifornia, Riverside, A 92521, USA Phone: 1 (951) Fax: 1 (951) zaera@ucr.edu 1 Dept. hemistry, Harvard University ambridge, MA ALD International onference Boston, June 28,
3 Introduction Atomic Layer Deposition ALD: Separate chemistry into two self-limiting and complementary reactions for more control H H H2 H H H 2 H 2 H H H 2 H2 H H 2 H opper Acetamidinate: Promising ALD precursor F. Zaera, J. Mater. hem., 18, (2008). 2
4 Amidinate Thermal hemistry Stepwise Decomposition, TPD on 220 K Molecular desorption 300 K s But H (H3 )=H 405 K Additional dehydrogenation Acetonitrile, amido group? 480 K β-hydride elimination to butene Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater., 22(2), (2010). Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 3
5 Amidinate Thermal hemistry Dimer Dissociation upon Adsorption H 2 H 2 H H H H 2 H H 2 < 150 K Dissociative adsorption H2 H 2 H H Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 4
6 Amidinate Thermal hemistry First Bond Dissociation, T ~ 200 K H 2 H 2 H H bond scission 200 K 3 H 2 H H H H H Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 5
7 Amidinate Thermal hemistry -sec-butylacetamidine Formation Molecular Desorption -sec-butylacetamidine H 2 3 H 2 H H H H (ads) 300 K +H 310 K 3 H 2 H H H H H Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 6
8 Amidinate Thermal hemistry Reduction ev ev opper reduction occurs as -secbutylacetamide desorbs K ev ev Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 7
9 Amidinate Thermal hemistry High Temperature onversion, 1s and 1s XPS ev ev ev ev H H 2 H 400 K Acetonitrile H ev ev H = H M. Xu, H. Tiznado, B.-. Kang, M. Bouman, I. Lee, F. Zaera, J. Kor. Phys. Soc., 51(3), (2007). Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 8
10 Amidinate Thermal hemistry Butene Formation and Further Dehydrogenation Butene H=H H K 405 K Acetonitrile = H 2 H H Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). 9
11 Amidinate Thermal hemistry Proposed Mechanism H 2 H 2 H H H H 2 H H 2 H2 H 2 H H Dissociative adsorption H 2 < 150 K (ads) Several intermediates form vs. T Some may desorb molecularly, but by ~ 480 K dehydrogenation is irreversible -sec butylacetamidine H 300 K H 2 H H 310 K K H K H H H H H ~500 K (ads) (ads) (ads) (?) = H 2 H 3 (?) 405 K Acetonitrile opper reduction (I) (0) Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). Butene H=H 480 K H H 2 H 10
12 Amidinate Uptake Effect of Temperature and Hydrogen Fast and continuous uptake above 460 K. Possible VD. Deposition of impurities. Butene desorption Extensive dehydrogenation Uptake past monolayer above 400 K Acetonitrile formation o uptake below 300 K -sec-butylacetamidine desorption o appreciable changes seen with hydrogen surface presaturation Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater., 22(2), (2010). 11
13 Amidinate Uptake Growth Rate, LEIS i Θ = 0.85 Saturation at ~ 15 L Some surface uncovered upon annealing ~ 3 ycles/ ML in ALD mode Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater., 22(2), (2010). 12
14 Amidinate Thermal hemistry Proposed Mechanism H 2 H 2 H H H H 2 H H 2 H2 H 2 H H Dissociative adsorption H 2 < 150 K (ads) Several intermediates form vs. T Some may desorb molecularly, but by ~ 480 K dehydrogenation is irreversible -sec butylacetamidine H 300 K H 2 H H 310 K K H K H H H H H ~500 K (ads) (ads) (ads) (?) = H 2 H 3 (?) 405 K Acetonitrile opper reduction (I) (0) Q. Ma, H. Guo, R. G. Gordon, F. Zaera, hem. Mater. (2011). Butene H=H 480 K H H 2 H 13
Surface Chemistry of Copper Precursors
Surface hemistry of opper Precursors in onnection with Atomic Layer Deposition (ALD) Processes Qiang Ma, Roy G. Gordon 1, and Dept. hemistry, University of alifornia, Riverside, A 92521, USA Phone: 1 (951)
More informationSurface Chemistry of Copper(I) Acetamidinates in Connection with Atomic Layer Deposition (ALD) Processes
Surface Chemistry of Copper(I) Acetamidinates in Connection with Atomic Layer Deposition (ALD) Processes The Harvard community has made this article openly available. Please share how this access benefits
More informationThermal Chemistry of Copper Acetamidinate ALD Precursors on
Thermal Chemistry of Copper Acetamidinate ALD Precursors on Silicon Oxide Surfaces Studied by XPS Yunxi Yao and Francisco Zaera* Department of Chemistry, University of California, Riverside, CA 92521,
More informationVoc impact of orientation-dependent x in anisotropic PV absorbers.
Voc impact of orientation-dependent x in anisotropic PV absorbers The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters Citation Chakraborty,
More information* Corresponding authors:
Mechanism of Olefin Hydrogenation Catalysis Driven by Palladium-Dissolved Hydrogen Satoshi Ohno,*, Markus Wilde,*, Kozo Mukai, Jun Yoshinobu, and Katsuyuki Fukutani Institute of Industrial Science, The
More informationEffect of the Nature of the Substrate on the Surface Chemistry of Atomic
Effect of the Nature of the Substrate on the Surface Chemistry of Atomic Layer Deposition Precursors Yunxi Yao, 1 Jason P. Coyle, 2 Seán T. Barry, 2 and Francisco Zaera 1,* 1 Department of Chemistry, University
More informationSupporting Information
Supporting Information Yao et al. 10.1073/pnas.1416368111 Fig. S1. In situ LEEM imaging of graphene growth via chemical vapor deposition (CVD) on Pt(111). The growth of graphene on Pt(111) via a CVD process
More informationThe Route to Better Catalysts: From Surface Science to Nanotechnology
The Route to Better Catalysts: From Surface Science to Nanotechnology by University of California Riverside, CA 92521, USA Phone: 1 (951) 827-5498 Fax: 1 (951) 827-3962 Email: zaera@ucr.edu http://www.zaera.chem.ucr.edu
More informationAcidic Water Monolayer on Ruthenium(0001)
Acidic Water Monolayer on Ruthenium(0001) Youngsoon Kim, Eui-seong Moon, Sunghwan Shin, and Heon Kang Department of Chemistry, Seoul National University, 1 Gwanak-ro, Seoul 151-747, Republic of Korea.
More informationAdsorption and Reaction of ortho-carborane on Pt(111)
Adsorption and Reaction of ortho-carborane on Pt(111) Final Report David Siap August 3, 2006 REU Program Advisors: Professor Trenary Aashani Tillekaratne University of Illinois at Chicago Department of
More informationTransition State for Alkyl Group Hydrogenation on Pt(111)
Published on Web 06/04/2008 Transition State for Alkyl Group Hydrogenation on Pt(111) Pingping Ye and Andrew J. Gellman*,,, Departments of Chemistry and Chemical Engineering, Carnegie Mellon UniVersity,
More informationThe Surface Chemistry of Propylene, 1-Iodopropane, and 1,3-Diiodopropane on MoAl Alloy Thin Films Formed on Dehydroxylated Alumina
J. Phys. Chem. B 2006, 110, 12555-12571 12555 The Surface Chemistry of Propylene, 1-Iodopropane, and 1,3-Diiodopropane on MoAl Alloy Thin Films Formed on Dehydroxylated Alumina Feng Gao, Yilin Wang, and
More informationNanoEngineering of Hybrid Carbon Nanotube Metal Composite Materials for Hydrogen Storage Anders Nilsson
NanoEngineering of Hybrid Carbon Nanotube Metal Composite Materials for Hydrogen Storage Anders Nilsson Stanford Synchrotron Radiation Laboratory (SSRL) and Stockholm University Coworkers and Ackowledgement
More informationTPD-MS. Photocatalytic Studies Using Temperature Programmed Desorption Mass Spectrometry (TPD-MS) APPLICATION NOTE NOTE
TPD-MS APPLICATION NOTE NOTE Photocatalytic Studies Using Temperature Programmed Desorption Mass Spectrometry (TPD-MS) Thermal analysis consists of many techniques for the exploration of the physical properties
More informationSurface Chemistry and Reaction Dynamics of Electron Beam Induced Deposition Processes
Surface Chemistry and Reaction Dynamics of Electron Beam Induced Deposition Processes e -? 2 nd FEBIP Workshop Thun, Switzerland 2008 Howard Fairbrother Johns Hopkins University Baltimore, MD, USA Outline
More informationSurface chemical processes of CH 2 =CCl 2 on Si(111) 7 7 mediated by low-energy electron and ion irradiation*
Surface chemical processes of CH 2 =CCl 2 on Si(111) 7 7 mediated by low-energy electron and ion irradiation* Z. He, X. Yang and K. T. Leung Department of Chemistry University of Waterloo Waterloo, Ontario
More informationC-N Coupling in Reactions between Atomic Nitrogen and Ethylene on Rh(111) van Hardeveld, R.M.; van Santen, R.A.; Niemantsverdriet, J.W.
C-N Coupling in Reactions between Atomic Nitrogen and Ethylene on Rh(111) van Hardeveld, R.M.; van Santen, R.A.; Niemantsverdriet, J.W. Published in: Journal of Physical Chemistry B DOI: 10.1021/jp970525m
More informationThe Transition State for Surface-Catalyzed Dehalogenation: C I Cleavage on Pd(111)
Journal of Catalysis 203, 41 50 (2001) doi:10.1006/jcat.2001.3310, available online at http://www.idealibrary.com on The Transition State for Surface-Catalyzed Dehalogenation: C I Cleavage on Pd(111) Mark
More informationReaction of Tributyl Phosphite with Oxidized Iron: Surface and Tribological Chemistry
Langmuir 2004, 20, 7557-7568 7557 Reaction of Tributyl Phosphite with Oxidized Iron: Surface and Tribological Chemistry Feng Gao, Octavio Furlong, Peter V. Kotvis, and Wilfred T. Tysoe* Department of Chemistry
More informationDetermining the Elastic Modulus and Hardness of an Ultrathin Film on a Substrate Using Nanoindentation
Determining the Elastic Modulus and Hardness of an Ultrathin Film on a Substrate Using Nanoindentation The Harvard community has made this article openly available. Please share how this access benefits
More informationMethanol on Co(0001): XPS, TDS, WF and LEED results
Surface Science 598 (2005) 128 135 www.elsevier.com/locate/susc Methanol on Co(0001): XPS, TDS, WF and LEED results K. Habermehl-Ćwirzeń a,b, *, J. Lahtinen a, P. Hautojärvi a a Laboratory of Physics,
More informationAniline hydrogenolysis on nickel: effects of surface hydrogen and surface structure
Catalysis Letters 34 (1995) 365-374 365 Aniline hydrogenolysis on nickel: effects of surface hydrogen and surface structure Scan X. Huang, Daniel A. Fischer a and John L. Gland 1 Department of Chemistry,
More informationDESIGN OF PRECURSORS FOR ALD
DESIG OF PRECURSORS FOR ALD Roy G. Gordon Cambridge, MA USA Jean-Sébastien Lehn, Huazhi Li, Qing Min Wang and Deo V. Shenai Advanced Thin-Film Technologies Group Rohm and Haas Electronic Materials orth
More informationHydrogenation of Single Walled Carbon Nanotubes
Hydrogenation of Single Walled Carbon Nanotubes Anders Nilsson Stanford Synchrotron Radiation Laboratory (SSRL) and Stockholm University Coworkers and Ackowledgement A. Nikitin 1), H. Ogasawara 1), D.
More informationr(equivalent): A Simple Effect Size Indicator
r(equivalent): A Simple Effect Size Indicator The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters Citation Rosenthal, Robert, and
More informationSimulating mechanism at the atomic-scale for atomically precise deposition and etching
SEMICON TechArena session on Advanced Materials 14 November 2017 Simulating mechanism at the atomic-scale for atomically precise deposition and etching Simon D. Elliott & Ekaterina Filatova simon.elliott@tyndall.ie
More informationCarbon Nanotubes as Future Energy Storage System
Carbon Nanotubes as Future Energy Storage System V Vasu, D Silambarasan To cite this version: V Vasu, D Silambarasan. Carbon Nanotubes as Future Energy Storage System. Mechanics, Materials Science Engineering
More informationVapor Phase Doping with N-type Dopant into Silicon by Atmospheric Pressure Chemical Vapor Deposition
495 10.1149/1.2986806 The Electrochemical Society Vapor Phase Doping with N-type Dopant into Silicon by Atmospheric Pressure Chemical Vapor Deposition Shotaro Takeuchi, Ngoc Duy Nguyen, Frederik Leys,
More informationAdsorption of hydrogen on clean and modified magnesium films
Downloaded from orbit.dtu.dk on: Apr 30, 2018 Adsorption of hydrogen on clean and modified magnesium films Johansson, Martin; Ostenfeld, Christopher Worsøe; Chorkendorff, Ib Published in: Physical Review
More informationElectronic Supplementary Information β-ketoiminato-based Copper(II) Complexes as CVD. Precursors for Copper and Copper Oxide Layer.
Electronic Supplementary Material (ESI) for Dalton Transactions. This journal is The Royal Society of Chemistry 2018 Electronic Supplementary Information β-ketoiminato-based Copper(II) Complexes as CVD
More informationSupplementary Information
Supplementary Information Supplementary Figure S1: Structure and composition of Teflon tape. (a) XRD spectra of original Teflon tape and Teflon tape subjected to annealing at 150 o C under Ar atmosphere.
More informationSupporting Information
Electronic Supplementary Material (ESI) for Physical Chemistry Chemical Physics. This journal is the Owner Societies 2014 Supporting Information A direct Fe-O coordination at FePc/MoO x interface investigated
More informationBimetallic ruthenium-copper nanoparticles embedded in. mesoporous carbon as an effective hydrogenation catalyst
Supporting Information Bimetallic ruthenium-copper nanoparticles embedded in mesoporous carbon as an effective hydrogenation catalyst Jiajia Liu, *a Li Li Zhang, b Jiatao Zhang, a Tao Liu, c and X. S.
More informationSoftware Contracts for Security
Software Contracts for Security The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters Citation Moore, Scott David. 2016. Software Contracts
More informationPlasma Etching: Atomic Scale Surface Fidelity and 2D Materials
1 Plasma Etching: Atomic Scale Surface Fidelity and 2D Materials Thorsten Lill, Keren J. Kanarik, Samantha Tan, Meihua Shen, Alex Yoon, Eric Hudson, Yang Pan, Jeffrey Marks, Vahid Vahedi, Richard A. Gottscho
More informationAmmonia adsorption on Zr(0001): effect of electron bombardment on hydrogen production
SURFACE AND INTERFACE ANALYSIS Surf. Interface Anal. 2002; 33: 945 949 Published online in Wiley InterScience (www.interscience.wiley.com). DOI: 10.1002/sia.1475 Ammonia adsorption on Zr(0001): effect
More informationSUPPLEMENTARY INFORMATION
SUPPLEMENTARY INFORMATION Using first principles to predict bimetallic catalysts for the ammonia decomposition reaction Danielle A. Hansgen, Dionisios G. Vlachos, Jingguang G. Chen SUPPLEMENTARY INFORMATION.
More informationIV.D.2 Hydrogen Storage Materials for Fuel Cell-Powered Vehicles
IV.D.2 Hydrogen Storage Materials for Fuel Cell-Powered Vehicles Andrew Goudy Delaware State University 2 N. Dupont Highway Dover, DE 99 Phone: (32) 857-6534 Email: agoudy@desu.edu DOE Managers Ned Stetson
More informationPathway and Kinetic Analysis on the Propyl Radical + O2 Reaction System
URL-J-126375 Rev. 1 PREPRINT Pathway and Kinetic Analysis on the Propyl Radical + 2 Reaction System J.W. Bozzelli W.J. Pitz This paper was prepared for submittal to the Fourth International onference on
More informationSupporting Information
Supporting Information Direct Chemical Vapor Deposition-Derived Graphene Glasses Targeting Wide Ranged Applications Jingyu Sun, Yubin Chen, Manish Kr. Priydarshi, Zhang Chen, Alicja Bachmatiuk,, Zhiyu
More informationSelective collision-induced desorption: Measurement of the -bonded C 2 H 4 binding energy on Ptˆ111 precovered with atomic oxygen
Selective collision-induced desorption: Measurement of the -bonded C 2 H 4 binding energy on Ptˆ111 precovered with atomic oxygen D. Velic and Robert J. Levis Department of Chemistry, Wayne State University,
More informationInteraction of Hydrogen on a Lanthanum hexaboride (111) Surface Jenna Cameli, Aashani Tillekaratne, Michael Trenary Department of Chemistry,
Interaction of Hydrogen on a Lanthanum hexaboride (111) Surface Jenna Cameli, Aashani Tillekaratne, Michael Trenary Department of Chemistry, University of Illinois at Chicago, Chicago, IL 60607 1 Abstract
More informationSurface spectroscopic studies of the deposition of TiN thin films from tetrakis-(dimethylamido)-titanium and ammonia
Surface spectroscopic studies of the deposition of TiN thin films from tetrakis-(dimethylamido)-titanium and ammonia J. S. Corneille, P. J. Chen, C. M. Truong, W. S. Oh, and D. W. Goodman a) Department
More informationAtomically Resolved Single-Walled Carbon Nanotube Intramolecular Junctions
Atomically Resolved Single-Walled Carbon Nanotube Intramolecular Junctions The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters Citation
More informationSpectral observation of conversion between ionized vs. non-ionized protoncoupled electron transfer interfaces
Spectral observation of conversion between ionized vs. non-ionized protoncoupled electron transfer interfaces The Harvard community has made this article openly available. Please share how this access
More informationSurface Chemistry of Alanine on Ni{111} Supporting Information
S1 Surface Chemistry of Alanine on Ni{111} Richard E. J. Nicklin 1, Alix Cornish 1, Andrey Shavorskiy 2, Silvia Baldanza 1, Karina Schulte 3, Zhi Liu 2, Roger A. Bennett 1, Georg Held 1,4 1 Department
More informationThe Adsorption and Decomposition of C 2 H 4 on Ru(001): A Combined TPR and Work Function Change Study
J. Phys. Chem. B 2000, 104, 3355-3363 3355 The Adsorption and Decomposition of C 2 H 4 on Ru(001): A Combined TPR and Work Function Change Study T. Livneh*, and M. Asscher Department of Physical Chemistry
More informationAdsorption and reaction of 1,3-butadiene on Pt(1 1 1) and Sn/Pt(1 1 1) surface alloys
Surface Science 572 (2004) 261 268 www.elsevier.com/locate/susc Adsorption and reaction of 1,3-butadiene on Pt(1 1 1) and Sn/Pt(1 1 1) surface alloys Haibo Zhao, Bruce E. Koel * Department of Chemistry,
More informationSupporting Information. for. Angew. Chem. Int. Ed. Z Wiley-VCH 2003
Supporting Information for Angew. Chem. Int. Ed. Z52074 Wiley-VCH 2003 69451 Weinheim, Germany Kinetic and Thermodynamic Control via Chemical Bond Rearrangement on Si(001) Surface Chiho Hamai, Akihiko
More informationLaser-induced photochemistry of methane on Pt(111): Excitation mechanism and dissociation dynamics
Laser-induced photochemistry of methane on Pt(111): Excitation mechanism and dissociation dynamics Yoshiyasu Matsumoto, Yuri A. Gruzdkov, a) Kazuo Watanabe, and Kyoichi Sawabe Institute for Molecular Science,
More informationFormic acid electro-synthesis from carbon dioxide in a room temperature ionic liquid
Supporting Information: Formic acid electro-synthesis from carbon dioxide in a room temperature ionic liquid Benjamin C. M. Martindale and Richard G. Compton a * Department of Chemistry, Physical and Theoretical
More informationOn adsorption of aluminium and methyl groups on silica for TMA/H 2 O process in atomic layer deposition of aluminium oxide nano layers
Bull. Mater. Sci., Vol. 33, No. 2, April 2010, pp. 97 102. Indian Academy of Sciences. On adsorption of aluminium and methyl groups on silica for TMA/H 2 O process in atomic layer deposition of aluminium
More informationMETHANOL OXIDATION OVER AU/ γ -AL 2 O 3 CATALYSTS
Bajopas Volume 2 Number 2 December, 29 Bayero Journal of Pure and Applied Sciences, 2(2): 149-154 Received: May, 29 Accepted: July, 29 METHANOL OXIDATION OVER AU/ γ -AL 2 O 3 CATALYSTS Abdullahi Nuhu Kano
More informationThe Transition State for Metal-Catalyzed Dehalogenation: C-I Bond Cleavage on Ag(111)
1440 J. Am. Chem. Soc. 2001, 123, 1440-1448 The Transition State for Metal-Catalyzed Dehalogenation: C-I Bond Cleavage on Ag(111) Mark T. Buelow and Andrew J. Gellman* Contribution from the Department
More informationCO and N2 differential depletion in prestellar cores: Experimental study of N2 desorption induced by the CO presence on ices
CO and N2 differential depletion in prestellar cores: Experimental study of N2 desorption induced by the CO presence on ices T.Nguyen, S. Baouche, E.Congiu, H.Chaabouni, L.Pagani, and F.Dulieu LERMA Lamap,
More informationJ. R Creighton and C. M. Truong Org. 1126, MS 0601 P.O. Box 5800 Sandia National Laboratories Albuquerque, NM
Fundamental Surface Chemistry of GaAs OMVPE J. R Creighton and C. M. Truong Org. 26, MS 060 P.O. Box 5800 Sandia National Laboratories Albuquerque, NM 8785060 Organometallic and hydride compounds are widely
More informationExploiting pattern transformation to tune phononic band gaps in a two-dimensional granular crystal
Exploiting pattern transformation to tune phononic band gaps in a two-dimensional granular crystal The Harvard community has made this article openly available. Please share how this access benefits you.
More informationINTERACTION OF CARBON MONOXIDE WITH CLEAN AND OXYGEN COVERED Cu( 11 I)-Ni SURFACE ALLOYS
Applications of Surface Science 20 (1984) l-12 North-Holland. Amsterdam INTERACTION OF CARBON MONOXIDE WITH CLEAN AND OXYGEN COVERED Cu( 11 I)-Ni SURFACE ALLOYS C.M.A.M. MESTERS *, A. DE KOSTER, O.L.J.
More informationA Game-Theoretic Analysis of Games with a Purpose
A Game-Theoretic Analysis of Games with a Purpose The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters. Citation Published Version
More informationChapter 7. Surface reactivity: geometry and electronic structure
146 Chapter 7. Surface reactivity: geometry and electronic structure 7.1 Introduction As described in previous chapters, the Ir(210) surface structure can be modified at will and in situ: the atomically
More informationUnderstanding the growth mechanism of graphene on Ge/Si(001) surfaces
Supplementary material for the manuscript: Understanding the growth mechanism of graphene on Ge/Si(001) surfaces J. Dabrowski, 1 G. Lippert, 1 J. Avila, 2 J. Baringhaus, 3 I. Colambo, 4 Yu. S. Dedkov,
More informationAtomic processes during Cl supersaturation etching of Si(100)-(2Ã 1)
Atomic processes during Cl supersaturation etching of Si(100)-(2Ã 1) C. M. Aldao,* Abhishek Agrawal, R. E. Butera, and J. H. Weaver Department of Materials Science and Engineering, University of Illinois
More informationSurface Reactions of Atomic Hydrogen with Ge(100) in Comparison with Si(100)
Appl. Sci. Converg. Technol. 26(6): 174-178 (2017) http://dx.doi.org/10.5757/asct.2017.26.6.174 Research Paper Surface Reactions of Atomic Hydrogen with Ge(100) in Comparison with Si(100) Sam Keun Jo*
More informationGAS-SURFACE INTERACTIONS
Page 1 of 16 GAS-SURFACE INTERACTIONS In modern surface science, important technological processes often involve the adsorption of molecules in gaseous form onto a surface. We can treat this adsorption
More informationGeneration and Reaction of Vinyl Groups on a Cu(100) Surface
J. Phys. Chem. 1996, 100, 12431-12439 12431 Generation and Reaction of Vinyl Groups on a Cu(100) Surface Michael X. Yang, Joseph Eng, Jr., Phillip W. Kash, George W. Flynn, and Brian E. Bent* Department
More informationEvidence for partial dissociation of water on flat MgO(1 0 0) surfaces
6 February 2002 Chemical Physics Letters 352 (2002) 318 322 www.elsevier.com/locate/cplett Evidence for partial dissociation of water on flat MgO(1 0 0) surfaces Y.D. Kim a, R.M. Lynden-Bell b, *, A. Alavi
More informationEnantioselective decomposition of chiral alkyl bromides on Cu(643) R&S : Effects of moving the chiral center
Surface Science 600 (2006) 2823 2829 www.elsevier.com/locate/susc Enantioselective decomposition of chiral alkyl bromides on Cu(643) R&S : Effects of moving the chiral center D.M. Rampulla, A.J. Gellman
More informationEnantioselective Separation on a Naturally Chiral Surface
Published on Web 10/26/2004 Enantioselective Separation on a Naturally Chiral Surface Joshua D. Horvath, Anjanette Koritnik, Preeti Kamakoti,, David S. Sholl,, and Andrew J. Gellman*, Contribution from
More informationCH 3 CH 2. OH, CD 3 CD 2 OD, and CF 3 CH 2 OH Decomposition on ZnO Introduction. Aaron Reinicker 1 James B. Miller. Andrew J.
Top Catal (15) 58:613 6 DOI 1.17/s11-15-3-z ORIGINAL PAPER CH 3 CH OH, CD 3 CD OD, and CF 3 CH OH Decomposition on ZnO 11 Aaron Reinicker 1 James B. Miller 1 Wooseok Kim Kijung Yong Andrew J. Gellman 1
More informationThe surface chemistry of ethylene adsorbed on Mo(100), oxygen-covered Mo(100) and MoO 2
surface science ELSEVIER Surface Science 383 (1997) 57 68 The surface chemistry of ethylene adsorbed on Mo(100), oxygen-covered Mo(100) and MoO 2 G. Wu, B. Bartlett, W.T. Tysoe * Department of Chemistry
More informationEffect of Electric Field on Condensed-Phase Molecular Systems. II. Stark Effect on the Hydroxyl Stretch Vibration of Ice
Effect of Electric Field on Condensed-Phase Molecular Systems. II. Stark Effect on the Hydroxyl Stretch Vibration of Ice Sunghwan Shin, Hani Kang, Daeheum Cho, Jin Yong Lee, *, and Heon Kang *, Department
More informationarxiv:cond-mat/ v1 [cond-mat.mtrl-sci] 23 May 2001
CO oxidation on a single Pd atom supported on magnesia arxiv:cond-mat/0105460v1 [cond-mat.mtrl-sci] 23 May 2001 S. Abbet, 1 U. Heiz, 2 H. Häkkinen 3 and U. Landman 3 1 Université de Lausanne, Institut
More informationFormation of clean dimers during gas-source growth of Si(001)
Formation of clean dimers during gas-source growth of Si(001) D.R.Bowler Department of Physics and Astronomy, University College London, Gower Street, London WC1E 6BT, UK (Dated: October 18, 2002) Elevated
More informationRole of Re and Ru in Re Ru/C Bimetallic Catalysts for the
Role of Re and Ru in Re Ru/C Bimetallic Catalysts for the Aqueous Hydrogenation of Succinic Acid Xin Di a, Chuang Li a, Bingsen Zhang b, Ji Qi a, Wenzhen Li c, Dangsheng Su b, Changhai Liang a, * a Laboratory
More informationDirect Synthesis of H 2 O 2 on AgPt Octahedra: The Importance of Ag-Pt Coordination for High H 2 O 2 Selectivity
Supporting Information Direct Synthesis of H 2 O 2 on AgPt Octahedra: The Importance of Ag-Pt Coordination for High H 2 O 2 Selectivity Neil M. Wilson, 1 Yung-Tin Pan, 1 Yu-Tsun Shao, 2 Jian-Min Zuo, 2
More informationArticle (peer-reviewed)
Title Decomposition of metal alkylamides, alkyls, and halides at reducible oxide surfaces: mechanism of 'clean-up' during atomic layer deposition of dielectrics onto III-V substrates Author(s) Klejna,
More informationHydrogenated Graphene
Hydrogenated Graphene Stefan Heun NEST, Istituto Nanoscienze-CNR and Scuola Normale Superiore Pisa, Italy Outline Epitaxial Graphene Hydrogen Chemisorbed on Graphene Hydrogen-Intercalated Graphene Outline
More informationPCCP PAPER. Electron induced reactions of surface adsorbed tungsten hexacarbonyl (W(CO) 6 ) Introduction
PAPER Cite this: Phys. Chem. Chem. Phys., 2013, 15, 4002 Electron induced reactions of surface adsorbed tungsten hexacarbonyl (W(CO) 6 ) Samantha G. Rosenberg, Michael Barclay and D. Howard Fairbrother*
More informationProcessing and Characterization of PMSSQ Based Materials for Nanoporous Low-K Dielectrics
Processing and Characterization of PMSSQ Based Materials for Nanoporous Low-K Dielectrics P. Lazzeri 1, L. Vanzetti 1, M. Bersani 1, M. Anderle 1, J.J. Park 2, Z. Lin 2,, R.M. Briber 2, G.W. Rubloff 2,
More informationThe effect of subsurface hydrogen on the adsorption of ethylene on Pd(1 1 1)
Surface Science 540 (2003) L600 L604 Surface Science Letters The effect of subsurface hydrogen on the adsorption of ethylene on Pd(1 1 1) D. Stacchiola, W.T. Tysoe * Department of Chemistry and Laboratory
More informationArticle (peer-reviewed)
Title Multiple proton diffusion and film densification in atomic layer deposition modeled by density functional theory Author(s) Shirazi, Mahdi; Elliott, Simon D. Publication date 2013-02-28 Original citation
More informationThermal decomposition mechanisms of tungsten nitride CVD precursors on Cu(111)
Surface Science 600 (2006) 743 754 www.elsevier.com/locate/susc Thermal decomposition mechanisms of tungsten nitride CVD precursors on Cu(111) Yaw-en Yang a,b, *, Jin-Bao u b,c, Jelin ang b,1, Yi-Feng
More informationCarbon Fluorine Reductive Elimination from a High Valent Palladium Fluoride
Carbon luorine Reductive Elimination from a High Valent Palladium luoride The Harvard community has made this article openly available. Please share how this access benefits you. Your story matters. Citation
More informationDehydrogenation of Liquid Organic Hydrogen Carriers In-situ Spectroscopic Studies
Dehydrogenation of Liquid Organic Hydrogen Carriers In-situ Spectroscopic Studies Chair of Physical Chemistry II C. Gleichweit, M. Amende, U. Bauer, S. Schernich, W. Zhao, M.P. A. Lorenz, O. Höfert, M.
More informationSeason Spotter: Using Citizen Science to Validate and Scale Plant Phenology from Near-Surface Remote Sensing
Season Spotter: Using Citizen Science to Validate and Scale Plant Phenology from Near-Surface Remote Sensing The Harvard community has made this article openly available. Please share how this access benefits
More informationCHEM53200: Lecture 5. Physisorption, Chemisorption & Catalysis
CHEM53200: Lecture 5 Physisorption, Chemisorption & Catalysis 1 2 3 Physical adsorption (physisorption) no barrier (not activated) fast vdw/dipole interactions weak (< 0.4 ev) always atomic/molecular reversible
More informationSelectivity in the initial C-H bond cleavage of n-butane on PdO(101)
Supporting Information for Selectivity in the initial C-H bond cleavage of n-butane on PdO(101) Can Hakanoglu (a), Feng Zhang (a), Abbin Antony (a), Aravind Asthagiri (b) and Jason F. Weaver (a) * (a)
More informationThe adsorption of acetic acid on Au/Pd(111) alloy surfaces
Surface Science 601 (2007) 1351 1357 www.elsevier.com/locate/susc The adsorption of acetic acid on Au/Pd(111) alloy surfaces Z. Li, F. Calaza, F. Gao, W.T. Tysoe * Department of Chemistry and Laboratory
More informationDynamic Equipment and Process Simulation for Atomic Layer Deposition Technology
Dynamic Equipment and Process Simulation for Atomic Layer Deposition Technology Wei Lei, Yuhong Cai, Laurent Henn-Lecordier and Gary W. Rubloff Department of Materials Science and Engineering and Institute
More informationProbing Enantioselectivity on Chirally Modified Cu(110), Cu(100), and Cu(111) Surfaces
pubs.acs.org/langmuir 2010 American Chemical Society Probing Enantioselectivity on Chirally Modified Cu(110), Cu(100), and Cu(111) Surfaces Wai Yeng Cheong, Ye Huang, Nikunj Dangaria, and Andrew J. Gellman*,,
More informationElectronic Processes on Semiconductor Surfaces during Chemisorption
Electronic Processes on Semiconductor Surfaces during Chemisorption T. Wolkenstein Translatedfrom Russian by E. M. Yankovskii Translation edited in part by Roy Morrison CONSULTANTS BUREAU NEW YORK AND
More informationChapter 3. Distinguishing between Reaction Intermediates and. Spectators: A Kinetic Study of Acetone Oxidation Using
Chapter 3 Distinguishing between Reaction Intermediates and Spectators: A Kinetic Study of Acetone Oxidation Using Ozone on a Silica-Supported Manganese Oxide Catalyst 3.1 Introduction This chapter concentrates
More informationMicrowave Synthesis of Monodisperse TiO 2 Quantum Dots and Enhanced Visible-Light Photocatalytic Properties
2014 3rd International Conference on Environment Energy and Biotechnology IPCBEE vol.70 (2014) (2014) IACSIT Press, Singapore DOI: 10.7763/IPCBEE. 2014. V70. 28 Microwave Synthesis of Monodisperse TiO
More informationEfficient Synthesis of Ethanol from CH 4 and Syngas on
Efficient Synthesis of Ethanol from CH 4 and Syngas on a Cu-Co/TiO 2 Catalyst Using a Stepwise Reactor Zhi-Jun Zuo 1, Fen Peng 1,2, Wei Huang 1,* 1 Key Laboratory of Coal Science and Technology of Ministry
More informationDesigning Graphene for Hydrogen Storage
Designing Graphene for Hydrogen Storage Stefan Heun NEST, Istituto Nanoscienze-CNR and Scuola Normale Superiore Pisa, Italy Outline Introduction to Hydrogen Storage Epitaxial Graphene Hydrogen Storage
More informationRaman studies on potential hydrogen storage materials
Raman studies on potential hydrogen storage materials The Hydrogen & Fuel Cell Researcher Conference University of Birmingham 17 th December 2013 Daniel Reed, David Book School of Metallurgy and Materials
More informationTable 1: Residence time (τ) in seconds for adsorbed molecules
1 Surfaces We got our first hint of the importance of surface processes in the mass spectrum of a high vacuum environment. The spectrum was dominated by water and carbon monoxide, species that represent
More information(Preeti Aghalayam, Sep 2011)
(Preeti Aghalayam, Sep 2011) Adsorbed States As A approaches the catalyst surface, the PE of the system goes through a minimum. Potential Energy (system) ΔH c ΔH p Physisorption vs. Chemisorption A + Catalyst
More informationWeek of July 23, 2012
Week of July 23, 2012 CBE In the News: Please join me in congratulating TERRY PAPOUTSAKIS, who has been chosen to receive the 2012 James E. Bailey Award from the Society of Biological Engineering of the
More informationThermal decomposition reactions of acetaldehyde and acetone on Si(100)
University of Nebraska - Lincoln DigitalCommons@University of Nebraska - Lincoln Marjorie A. Langell Publications Published Research - Department of Chemistry May 1997 Thermal decomposition reactions of
More information